The pill test is the US federal flammability test for carpets and rugs. A methenamine tablet is lit on each of eight specimens, and the product passes if at least seven of the eight do not char to within one inch of the edge of the hole in the steel frame. Large carpets and rugs are covered by 16 CFR 1630 and small ones by 16 CFR 1631, and ASTM D2859 is the ASTM test method for the same kind of tablet test on finished textile floor coverings.
Why a hotel needs it
The pill test is a minimum for carpets and rugs sold in the United States, not a hotel specific standard. It answers a narrow question: what happens if a small burning object, such as a dropped match or an ember, lands on the rug. It does not measure flame spread under radiant heat in a corridor, which is the job of ASTM E648.
Hotel specifications therefore usually ask for both: the pill test as the floor everywhere, and a radiant panel class for corridors and exits where the code requires one.
Large or small: 1630 or 1631
| 16 CFR 1630 | 16 CFR 1631 | |
|---|---|---|
| Also known as | FF 1-70 | FF 2-70 |
| Covers | Carpets and rugs with one dimension greater than 6 feet (1.83 m) and a surface area greater than 24 square feet (2.23 m²) | Carpets and rugs with no dimension greater than 6 feet and a surface area of 24 square feet or less |
| If the product fails | It may not be sold | It may be sold only with a permanent warning label |
Carpet tiles and squares that are smaller than these limits but intended to be assembled into a larger installation are included in the large carpet standard. The definition also covers mats and hides of the defined sizes. Resilient floor coverings such as vinyl and linoleum are excluded.
For a hotel, most guest room and public area rugs are large carpets under 1630. Bath mats and small bedside rugs are often small carpets under 1631.
How the test works
The federal standard sets out each step.
- Eight specimens, each 9 by 9 inches, are cut from the carpet or rug.
- They are dried in a forced air oven at 105 °C for two hours, then cooled in a desiccator for at least an hour.
- Each specimen is placed in a draught protected test chamber under a metal flattening frame with a circular hole in its centre.
- A methenamine tablet is placed at the centre and ignited.
- When burning stops, the distance from the charred area to the edge of the hole is measured.
A specimen passes if the char does not reach within 1 inch (2.54 cm) of the edge of the hole at any point. The carpet passes if at least seven of the eight specimens pass.
ASTM D2859 describes a test for the flammability of finished textile floor covering materials exposed to a methenamine tablet under controlled laboratory conditions, for natural and man made fibres alike. Specifications often cite it alongside the federal parts. The legal requirement for products sold in the United States is the federal standard, so a report should reference 16 CFR 1630 or 1631 as well.
Labels and treated products
Small carpets that fail under 1631 may still be sold if they carry a permanent label reading: FLAMMABLE (FAILS U.S. DEPARTMENT OF COMMERCE STANDARD FF 2-70): SHOULD NOT BE USED NEAR SOURCES OF IGNITION. There is no equivalent option for large carpets. A hotel buyer should not accept a labelled small rug for a commercial interior without the fire consultant's agreement.
If a carpet or rug has had a fire retardant treatment, or contains treated fibres, it must be labelled with the letter T, and the specimens must be washed or laundered ten times by the prescribed method before testing. This is meant to show that the treatment survives cleaning. CPSC guidance notes that the laundering requirement is currently suspended for large carpets that use alumina trihydrate in the backing.
What the one of a kind exemption does and does not cover
The large carpet standard allows a one of a kind carpet or rug, such as an antique, an Oriental or a hide, to be excluded from testing under conditions set by the Consumer Product Safety Commission. This is sometimes misread as an exemption for handmade rugs in general. A hotel order of the same design repeated across many rooms is not a one of a kind product. Plan to test.
What tends to fail
CPSC staff note that untreated rugs which typically fail are shag or fluffy constructions and those with a polyurethane foam cushion layer. Long loose pile gives the small flame more fuel and more air. Low, dense wool constructions generally behave better, because wool is hard to ignite and tends to char, but the result belongs to the construction tested, not the fibre.
Certificates for imported rugs
CPSC requires a General Certificate of Conformity for general use carpets and rugs, based on a test of each product or a reasonable testing programme. For imported goods the importer is responsible for issuing it. Carpets intended primarily for children aged 12 and under need a Children's Product Certificate based on third party testing.
Checklist for hotel buyers
- Identify which rugs fall under 1630 and which under 1631, from the size schedule
- Ask for a report referencing the federal part, from an accredited laboratory
- Check the report describes the exact construction, backing and any treatment
- If treated, check the T label and the laundering step in the report
- Agree who issues the General Certificate of Conformity before shipment
- Do not rely on the one of a kind exemption for repeated designs
- Add ASTM E648 for corridors where the code requires a class
How Eastern Mills handles it
Eastern Mills manufactures hand tufted rugs, hand knotted and handloom rugs for hotels and exports to more than 30 countries. Construction is set per project, and testing to the project's named standard is arranged per order on the construction to be shipped. The hospitality page explains how hotel projects run, and the brief can be sent through contact.
Requirements vary by jurisdiction and project, and the project's fire engineer or code consultant decides which standards apply.
Frequently asked questions
Is the pill test enough for hotel corridors?
Usually not. Corridors and exits often need a critical radiant flux class under ASTM E648. The pill test is the minimum for all carpets and rugs sold in the United States.
Does every size of rug in an order need testing?
The test is on the construction, so one result can cover several sizes of the same construction. The size decides whether 1630 or 1631 applies.
Why are specimens dried before the test?
Moisture in the fibre slows burning. Oven drying puts every specimen in the same, demanding condition.
Do wool rugs pass automatically?
No. Wool helps, but pile height, density, backing and cushion all affect the result.